AVIC Henan Hong is a professional production and sales of honeycomb carbon, honeycomb activated carbon factory. The main products are: honeycomb carbon, honeycomb activated carbon, waterproof honeycomb activated carbon, water resistant honeycomb activated carbon, honeycomb activated carbon block, cylindrical honeycomb activated carbon, honeycomb shaped activated carbon, etc.. The company has always adhere to the "quality first, customer first, quality service, abide by the contract," the purpose, with a high-quality products, good reputation, high quality service, the best-selling products in more than and 30 provinces, municipalities and autonomous regions and exported to Japan, the United States and other countries. Wholeheartedly with the domestic and foreign merchants win-win cooperation, common development, create brilliant!
蜂窝活性炭生产方法 步是:褐煤或烟煤与焦煤分别破碎到小于2毫米(mm),然后按质量比褐煤或烟煤∶焦煤为1∶0.2—0.5混合后,再研磨至74米(μm)以下,会得到混合均匀的煤粉。
蜂窝活性炭生产方法第二步是:1、沥青含量大于等于55%高温煤焦油预热至120—150℃;2、乳化剂水溶液的配制,在水中加入高温煤焦油质量的2—6%表面活性剂和高温煤焦油质量的0.5—2%的稳定剂,并预热至80—90摄氏度(℃)形成乳化剂水溶液,3、按质量比为高温煤焦油∶乳化剂水溶液=1∶0.3—0.7,在搅拌条件下,将高温煤焦油加入乳化剂水溶液中制成乳化煤焦油。
蜂窝活性炭生产方法第三步是:按质量比为煤粉∶乳化煤焦油∶水∶水溶性粘合剂∶润滑剂=34—57∶30—36∶6—29∶3—5∶2—3,将其加入捏合机当中搅拌均匀后,能够制成可塑性的煤泥。
蜂窝活性炭生产方法第四步是:可塑性煤泥经过真空练泥机或挤出成型机处理,使得煤泥混合均匀,然后在成型机中用60—100目的丝网中过滤除掉大颗粒物质。
蜂窝活性炭生产方法第五步:练泥处理后的煤泥加入装有蜂窝钢模具的挤出成型机中,进行成型,得到湿的蜂窝体。
蜂窝活性炭生产方法第六步:湿的蜂窝体干燥至水分低于2%;以惰性气体作为保护气,按升温速度3-5℃/min(摄氏度/分钟)加热到600—800℃,并且在此温度下炭化2—3个小时;然后按升温速度5—15℃/min(摄氏度/分钟)升温到750—850℃,用水蒸气活化3—15个小时,经过多道工艺终于制成蜂窝活性炭。